CN104119786A - Powder coating composition with effect of repelling insects and preparation method of powder coating composition - Google Patents

Powder coating composition with effect of repelling insects and preparation method of powder coating composition Download PDF

Info

Publication number
CN104119786A
CN104119786A CN201410391199.5A CN201410391199A CN104119786A CN 104119786 A CN104119786 A CN 104119786A CN 201410391199 A CN201410391199 A CN 201410391199A CN 104119786 A CN104119786 A CN 104119786A
Authority
CN
China
Prior art keywords
powder coating
pyrethroid
effect
fluorine
coating composition
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410391199.5A
Other languages
Chinese (zh)
Inventor
韩巧
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN201410391199.5A priority Critical patent/CN104119786A/en
Publication of CN104119786A publication Critical patent/CN104119786A/en
Pending legal-status Critical Current

Abstract

The invention discloses a powder coating composition with an effect of repelling insects and a preparation method of the powder coating composition. The powder coating composition is characterized by being prepared from the following components in percentage by weight: 20-30% of epoxy resin, 30-40% of polyester resin, 1-1.5% of a flatting agent, 0.3-0.5% of benzoin, 0.3-1% of polytetrafluoroethylene wax, 10-25% of titanium dioxide, 10-20% of barium sulfate and 0.1-1% of fluorine-containing pyrethroid. By selecting a safe, environment-friendly and long-acting insect repellant which is good in compatibility with raw materials in the powder coating formula, suitable for the powder coating production process and spraying process and free from side effects to product performance in production and use, the effect of repelling insects by the powder coating is realized by scientifically proportioning and adding a certain proportion of the repellant, and the coating can maintain a good coating performance and appearance.

Description

There is powder paint compositions of repel insects effect and preparation method thereof
Technical field
The present invention relates to a kind of powder coating, particularly a kind of powder coating of walking quickly and keeping away insect effect.The invention further relates to the preparation method of above-mentioned powder coating.
Background technology
Powder coating is a kind of important industrial coating, current powder coating is because of its environmental protection and energy saving, VOC free discharge, the features such as one-pass film-forming is pollution-free, free from extraneous odour, and film performance excellence is attractive in appearance have become the first-selected application mode of people's daily necessitiess such as household electrical appliance, light fixture, kitchen tackle, outdoor furniture.
And in people's daily life, be often subject to the invasions of the insects such as mosquitos and flies, cockroach, ant; in the gap of refrigerator and wall, often having cockroach occurs; the frequent search of food chip of ant in kitchen; insect can invade the inside of means of illumination, and requires great effort in cleaning globe glass lamp shade inside very much.
Therefore the powder coating that makes to be coated on these products has the effect of walking quickly and keeping away insect and people is lived significant.But because production technique and the spraying curing process of powder coating all need to complete under comparatively high temps, do not have in the market after high bake solidifies, still to possess and to walk quickly and keep away insect effect, and still can keep the coating products of its good coating property.
Summary of the invention
The present invention completes in order to solve above-mentioned deficiency of the prior art, the object of this invention is to provide a kind of powder paint compositions of walking quickly and keeping away insect effect that has, another object of the present invention is to provide a kind of preparation method with the powder paint compositions of walking quickly and keeping away insect effect, the present invention is good by selecting with powder coating formula Central Plains material compatibility, can be applicable to powder coating production technique and spraying coating process, in production and use, product performance are had no side effect, safety, environmental protection, long-acting wormer, the science being listed as by the ratio of filling a prescription certain is added, reach powder coating and walk quickly and keep away the effect of insect. and make coating can keep good coating property and outward appearance.
An object of the present invention is to provide a kind of powder paint compositions of walking quickly and keeping away worm effect that has, its concrete technical scheme is as described below:
There is a powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described composition comprises following component:
Further technical scheme, described in there is the powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described composition comprises following component:
Technical scheme further, described in there is the powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described composition comprises following component:
Further technical scheme of the present invention, wherein said have a powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described fluorine-containing pyrethroid is fluorine silicon pyrethroid or fluorine the third pyrethroid.
The present invention also provides a kind of preparation method with the powder paint compositions of walking quickly and keeping away insect effect, wherein according to above-mentioned each component concentration, take each component, then by vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and are fully stirred, churning time is 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate, fluorine-containing pyrethroid continues to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock is ground into powder.
The present invention adds the pyrethroid of fluoropolymer as wormer in formula, realizes the avoidance effect to insect.Pyrethroid is the broad spectrum pesticide that a class can be prevented and treated various pests, and its insecticidal toxicity improves 10~100 times than older generation sterilant as organochlorine, organophosphorus, amino formate.Pyrethroid has strong action of contace poison or fumigation action to insect, and its mechanism of action is to upset the normal physiological of insect nerve, makes it by excited, spasm death to benumbing.Pyrethroid is because consumption is little, working concentration is low, thus safer to people and animals, very little to the pollution of environment.Conventional pyrethroid temperature tolerance on market is generally 80 ℃, and powder coating temperature when producing reaches 120 ℃, when curing, temperature reaches 180 ℃ especially, we are by carrying out heatproof test and various technical screening in laboratory, discovery is in pyrethroid molecular chain after grafting fluorochemicals, the temperature tolerance of pyrethroid can arrive 200 ℃, and with powder coating in other starting material have very much good consistency, do not need existing machinery equipment in process of production, production technique is transformed.
By to the screening of fluorinated pyrethrin pesticide in the market, applicant's preferred four kinds of fluorine-containing pyrethroids in numerous sterilants carry out contrast experiment, it is extremely low that it has acute toxicity and chronic toxicity, without the feature of teratogenesis, carinogenicity risk, and has and anergy good with coating consistency.
Embodiment
Below in conjunction with embodiment and embodiment, powder coating of walking quickly and keeping away insect effect of the present invention is described in further detail.The effect that it should be noted that following examples is in order to illustrate further the present invention, and is not limitation of the present invention.
Embodiment 1:
According to embodiment in table 21, take each component, vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and fully stirred, churning time is 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate, tetrafluoro pyrethroid to continue to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock be ground into powder.Film forming after resulting powder is solidified by 200 ℃/10min on the thick tinplate of 0.5mm by electrostatic spraying, obtains model, tests its film forming properties, and tests other performance according to the GB providing in table.
Embodiment 2:
According to embodiment in table 22, take each component, vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and fully stirred, churning time is 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate, cyfluthrin pyrethroid to continue to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock be ground into powder.Film forming after resulting powder is solidified by 200 ℃/10min on the thick tinplate of 0.5mm by electrostatic spraying, obtains model, tests its film forming properties, and tests other performance according to the GB providing in table.
Embodiment 3:
According to embodiment in table 23, take each component, vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and fully stirred, churning time is 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate, fluorine the third pyrethroid to continue to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock be ground into powder.Film forming after resulting powder is solidified by 200 ℃/10min on the thick tinplate of 0.5mm by electrostatic spraying, obtains model, tests its film forming properties, and tests other performance according to the GB providing in table.It in table 1, is the result contrast of testing standard and embodiment 3.
Table 1
Embodiment 4
According to embodiment in table 24, take each component, vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and fully stirred, churning time is 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate, fluorine silicon pyrethroid to continue to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock be ground into powder.Film forming after resulting powder is solidified by 200 ℃/10min on the thick tinplate of 0.5mm by electrostatic spraying, obtains model, tests its film forming properties, and tests other performance according to the GB providing in table.
Embodiment 5
According to embodiment in table 25, take each component, vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and fully stirred, churning time is 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate to continue to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock be ground into powder.Film forming after resulting powder is solidified by 200 ℃/10min on the thick tinplate of 0.5mm by electrostatic spraying, obtains model, tests its film forming properties, and tests other performance according to the GB providing in table.
Disinsectization performance experimental technique
1, prepare two of the opening glasswares of long 50cm, wide 40cm, high 40cm;
2, the powder coating and the formula five powder coating samples that do not add any wormer that above-mentioned formula four are added to fluorine silicon pyrethroids spray respectively a block length 50cm, and the cold-rolled steel sheet of wide 20cm, thick 0.5mm is as experiment model mark formula four and formula five samples;
3, two models are placed in respectively to glassware bottom, make it occupy the general area in glass jar bottom;
4, two groups of each of China Formica rufas are placed in respectively in two experiment glass jars, observe ant active state, can find out that in the glass jar of placing fluorine silicon pyrethroid powder coating model, ant is all gathered in the side that cylinder bottom is not covered by model, place the random distribution shape of ant journey at the bottom of the glass jar of the powder coating model do not add wormer, at the bottom of glass jar and on model, all have distribution;
Repeat above-mentioned experimental procedure and Chinese Formica rufa is changed into other insects such as housefly, cockroach, piebald mosquito, bedbug, the powder coating model that can observe interpolation fluorine silicon pyrethroid has and significantly walks quickly and keeps away effect above-mentioned insect equally.
According to above test method, the product of embodiment 1-5 is tested, its result provides in table 2.
Table 2
From showing the experiment contrast of formula that other starting material consistencies are best in fluorine silicon pyrethroid or fluorine the third pyrethroid are filled a prescription with powder coating, the embodiment 5 that adds the embodiment 3,4 of fluorine silicon pyrethroid or fluorine the third pyrethroid 0.5% in experiment and do not add any sterilant shows basically identical appearance of film, gloss and mechanical property.From gel time, add fluorine silicon pyrethroid to formula in other materials not katalysis, do not need the original production process of powder coating to adjust.
Beneficial effect
Compared with prior art, because beneficial effect of the present invention is mainly: first provides a kind of coating composition of walking quickly and keeping away insect that has, and it possesses the stronger effect of walking quickly and keeping away insect; The second coating composition of the present invention is by selecting specific component, makes coating composition still have good coating property walk quickly and keep away more by force insect effect in the situation that having; The 3rd by choose reasonable components in coating compositions, makes pyrethroid and coating composition wherein have excellent compatibility, and does not affect and the reaction of participation system, high temperature resistant, thereby in coating production process, do not need existing machinery equipment, production technique is transformed, and has reduced cost.
Above-mentionedly only several specific embodiments in the present invention are illustrated; but can not be as protection scope of the present invention; every equivalence variation of having done according to the design spirit in the present invention or modification or equal proportion zoom in or out etc., all should think and fall into protection scope of the present invention.

Claims (5)

1. there is a powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described composition comprises following component:
2. there is according to claim 1 the powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described composition comprises following component:
3. according to claim 2 have a powder paint compositions of walking quickly and keeping away insect effect, it is characterized in that described composition comprises following component:
4. according to the powder paint compositions of walking quickly and keeping away insect effect that has described in the arbitrary claim of claim 1-3, it is characterized in that described fluorine-containing pyrethroid is fluorine silicon pyrethroid or fluorine the third pyrethroid.
5. according to having of claim 1 to 4, walk quickly and keep away the preparation method of the powder paint compositions of insect effect, it is characterized in that comprising the following steps:
By each component concentration, take each component, then vibrin, epoxy resin, flow agent, four kinds of components of titanium dioxide are put in mixing tank and fully stirred, churning time is about 300s, after stirring, add st-yrax, tetrafluoroethylene wax, barium sulfate, fluorine-containing pyrethroid to continue to stir 300s, then the raw material mixing is put in forcing machine and extruded, extruder temperature is set to first and extrudes 90 ℃, district, two extrude 95 ℃, district, by sheeter roller, be pressed into again the sheet stock of 1-10mm thickness, then by grinding machine, sheet stock be ground into Powdered finished product.
CN201410391199.5A 2014-08-10 2014-08-10 Powder coating composition with effect of repelling insects and preparation method of powder coating composition Pending CN104119786A (en)