Prior art keywords
self
coating
microcapsules
healing coating
healing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Abandoned
Application number
US11/789,811
Inventor
Larry D. Stephenson
Curtis Thies
Ashok Kumar
Srinivasan Sarangapani
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to US11/789,811 priority Critical patent/US20080152815A1/en
Publication of US20080152815A1 publication Critical patent/US20080152815A1/en
Abandoned legal-status Critical Current

Links

Images

Classifications

    • CCHEMISTRY; METALLURGY
    • C09DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09DCOATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D5/00Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
    • C09D5/08Anti-corrosive paints
    • C09D5/082Anti-corrosive paints characterised by the anti-corrosive pigment
    • C09D5/086Organic or non-macromolecular compounds
    • CCHEMISTRY; METALLURGY
    • C09DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09DCOATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D7/00Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
    • C09D7/40Additives
    • C09D7/48Stabilisers against degradation by oxygen, light or heat
    • CCHEMISTRY; METALLURGY
    • C09DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09DCOATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D7/00Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
    • C09D7/40Additives
    • C09D7/66Additives characterised by particle size
    • C09D7/69Particle size larger than 1000 nm
    • CCHEMISTRY; METALLURGY
    • C09DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09DCOATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D7/00Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
    • C09D7/40Additives
    • C09D7/70Additives characterised by shape, e.g. fibres, flakes or microspheres
    • BPERFORMING OPERATIONS; TRANSPORTING
    • B05SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05DPROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D5/00Processes for applying liquids or other fluent materials to surfaces to obtain special surface effects, finishes or structures
    • B05D5/005Repairing damaged coatings
    • CCHEMISTRY; METALLURGY
    • C08ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08KUse of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K9/00Use of pretreated ingredients
    • C08K9/10Encapsulated ingredients
    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10TTECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T428/00Stock material or miscellaneous articles
    • Y10T428/29Coated or structually defined flake, particle, cell, strand, strand portion, rod, filament, macroscopic fiber or mass thereof
    • Y10T428/2982Particulate matter [e.g., sphere, flake, etc.]
    • Y10T428/2984Microcapsule with fluid core [includes liposome]
    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10TTECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
    • Y10T428/00Stock material or miscellaneous articles
    • Y10T428/29Coated or structually defined flake, particle, cell, strand, strand portion, rod, filament, macroscopic fiber or mass thereof
    • Y10T428/2982Particulate matter [e.g., sphere, flake, etc.]
    • Y10T428/2984Microcapsule with fluid core [includes liposome]
    • Y10T428/2985Solid-walled microcapsule from synthetic polymer

Definitions

  • the present invention relates generally to coatings, in particular coatings that have been modified to provide a self-healing characteristic.
  • Microcapsules contain minute amounts of product for specialized delivery, often size, time or location critical. They may be obtained in diameters of less than 250 microns ( ⁇ ) and have been used in a variety of applications, from the pharmaceutical industry (delivery of drugs) to the textile industry (providing protective wear for HAZMAT workers).
  • microns
  • One example is U.S. Pat. No. 6,060,152, Fabric with Microencapsulated Breach Indication Coating, to Murchie, May 9, 2000.
  • the '152 patent describes a membrane incorporating a number of different microcapsules that alert to even the smallest compromise of the fabric comprising a protective suit such as may be worn by a HAZMAT worker or health professional.
  • the microcapsule and its contents may “deploy” before the coating is applied or, upon application, spontaneously deploy improperly, i.e., without a physical compromise of the coating such as abrasion or nicking. Further, unless the microcapsule is compatible with both its contents (the encapsulated repair compound) and its surrounds (the solvent), the “application” life of the resultant mixed product may be less than desirable.
  • the combination of one or more solvents and one or more solids may comprise a protective coating that would serve the purpose of protecting a substrate but not have the self-healing properties of the present invention.
  • This protective coating may be one of a number of commercially available products, to include primer paints, topcoat paints, “one coat” or “self-priming” paints, varnishes, lacquers, polyurethane finishes, shellacs, waxes, polishes, “one step” finishing preparations for wood, metal, or synthetic materials, and combinations thereof.
  • the paint primers may be: polyurethanes, oil-based enamels, enamel undercoater, latex acrylics, acrylic formulations and epoxy formulations.
  • topcoat and self-priming paints may be: polyurethanes, oil-based enamels, enamels, latex acrylics, acrylic formulations and epoxy formulations.
  • the microcapsules are added prior to application as a pre-specified percentage of the dry weight of the solids in the base coating at a pre-specified time prior to application of the self-healing coating.
  • the pre-specified percentage lies in the approximate range of 10 to 40% and the microcapsules are added within fourteen (14) days of application.
  • the pre-specified percentage is approximately 25% and the microcapsules are added when preparing the coating for application.
  • this microcapsule suitable for adding to available protective coatings to facilitate self-healing thereof after application and curing.
  • this microcapsule comprises a repair substance and a shell enclosing a volume containing the repair substance.
  • physical damage to the resultant coating ruptures the shell of the microcapsules in the vicinity of the rupture and deploys the repair substance into a volume (void) within the coating caused by the physical damage.
  • the shell of the microcapsule may be a sphere with an outer diameter preferably within the approximate range of 50 to 200 ⁇ . More preferably, the shell has an outer diameter greater than approximately 63 ⁇ . Most preferably, the shell has an outer diameter of approximately 150 ⁇ .
  • the shell of the microcapsule may be gelatin, or preferably urea formaldehyde (UF).
  • the repair substance contained therein may comprise film-forming compounds and corrosion inhibiting compounds.
  • the film-forming compounds may be any of: polybutenes, phenolics, phenolic varnishes, and combinations thereof.
  • the diluents may be any of: long chain polyester diluents, carrier diluents, and combinations thereof.
  • the corrosion inhibiting compounds may be any of: camphor; alkylammonium salt in xylene, commercially available as Ciba IRGACOR® 153 (anti-corrosion agent A); polyamine fatty acid in salt in ethanol, commercially available as Ciba IRGACOR® 287 (anti-corrosion agent B); and combinations thereof.
  • a method for producing a self-healing coating upon a substrate comprises: (a) providing a non-self healing coating; (b) providing microcapsules filled with a repair substance compatible with the non-self healing coating; (c) mixing the microcapsules into the non-self healing coating such that the microcapsules are fully wetted and interspersed evenly throughout the non-self healing coating; (d) applying the self-healing coating to the substrate by any of a number of means selected from the group consisting of: brushing, rolling, spraying, and combinations thereof; and (e) permitting the applied self-healing coating to cure prior to use of the substrate.
  • FIG. 1A is a micrograph typical of small gelatin microcapsules ( ⁇ 63 ⁇ diameter) as collapsed when immersed in wet polyurethane when investigated for possible use in the present invention.
  • FIG. 1B is a micrograph typical of medium gelatin microcapsules (63-150 ⁇ diameter) after two (2) hours immersion in wet polyurethane when investigated for possible use in the present invention.
  • FIG. 2B is a micrograph typical of large urea-formaldehyde (UF) microcapsules (>150 ⁇ diameter) deteriorating after four (4) weeks immersion in wet polyurethane when investigated for possible use in the present invention.
  • UF large urea-formaldehyde
  • FIG. 3 depicts a suggested mechanism for the collapse of microcapsules in wet coatings.
  • FIG. 4A is a micrograph showing the effect of burst UF microcapsules incorporated in applied coatings of the present invention in which a crack is induced in the coating.
  • FIG. 4B is a micrograph showing the effect of burst UF microcapsules incorporated in applied coatings of the present invention in which the coating has been scribed.
  • FIG. 5A depicts a cross section through a cube containing a single large microcapsule that may be used in a preferred embodiment of the present invention.
  • FIG. 5B depicts a cross section through the cube of FIG. 5A with a superimposed symmetric array of nine small microcapsules that fit in the same cube containing the large microcapsule of FIG. 5A .
  • FIG. 6 details the test results for the control and the three (3) self-healing coatings that may be employed as preferred embodiments of the present invention.
  • FIG. 7 depicts the relationship between impedance and frequency for both a control sample and a preferred embodiment of the present invention using data taken with Electrochemical Impedance Spectroscopy (EIS).
  • EIS Electrochemical Impedance Spectroscopy
  • FIG. 8 depicts the relationship between phase angle and frequency for both a control sample and a preferred embodiment of the present invention using data taken with EIS.
  • a preferred embodiment of the present invention provides a “self-healing” coating system that may be used for corrosion protection, such as on outdoor steel cabinet enclosures for electrical equipment.
  • Microcapsules in the form of microscopic spheres with a diameter of 50-200 ⁇ , and more preferably of 60-150 ⁇ diameter, are used to encapsulate “coating repairing” compounds as a means of effecting self-healing of the applied coating thus derived.
  • These microcapsules are fabricated for optimum dispersal into various coating formulations, e.g., paint, enabling release of the coating repairing or “self-healing” compounds. These compounds may comprise, at least in part, corrosion-inhibiting constituents.
  • Corrosion-inhibiting microcapsules may be used in coating systems to minimize damage caused by scratches or abrasions by releasing specially formulated chemicals that flow into the damaged areas forming thin films of corrosion protection.
  • self-healing coatings are fabricated by adding microcapsules containing at least one “self-healing” compound to commercially available paint primers. Paint primers may include those paints commercially termed “one coat” or “self-priming.” The microcapsules release the self-healing compound or compounds, most commonly as liquids, when the coating system is damaged. Urea formaldehyde (UF) microcapsules of 50-150 ⁇ in diameter have been added to primers with an applied thickness of 0.1 mm (0.004′′) to increase the coating service life by “self-healing” damaged areas. Verification of performance was conducted by accelerated corrosion testing on conventional coating systems using ASTM D 5894 and Electrochemical Impedance Spectroscopy (EIS). M.
  • EIS Electrochemical Impedance Spectroscopy
  • microcapsules Achieving timely and appropriate rupturing of microcapsules to be incorporated in applied coatings is crucial to developing and commercializing “self-healing” coatings. “Timely and appropriate rupturing” occurs, for example, when the applied coating is damaged physically or if cracks develop in the applied coating. Microcapsules may exhibit at least two major “improper rupturing” modes; viz., rupturing before the coating is applied to a surface and spontaneous rupturing on the surface of applied coatings prior to cracking or physical damage.
  • samples of each are bottled. Samples are extracted from each bottle and placed on glass slides. Initial optical micrographs of each are taken. After initial sampling, each bottle is tightly sealed. Optical micrographs of each sample are taken weekly over a period of four (4) weeks, and deterioration (if any) as a function of time is noted.
  • a listing of the types and quantities of tested microcapsules, designated as: small ( ⁇ 63 ⁇ ), medium (63-150 ⁇ ), and large (>150 ⁇ ), is shown in Table 1.
  • FIG. 1 Small gelatin microcapsules 101 (diameters less than 63 ⁇ ) failed to maintain structural integrity and self ruptured in polyurethane and other coatings in a few days.
  • a micrograph typical of collapsed small gelatin microcapsules 101 is shown in FIG. 1A .
  • medium (63-150 ⁇ ) gelatin microcapsules 102 maintain integrity somewhat longer than a few days.
  • large UF microcapsules 201 (diameter greater than 150 ⁇ ) maintained integrity for at least two (2) weeks.
  • FIG. 2B even the large UF microcapsules 201 began to collapse 202 and lose core material after four (4) weeks immersion in wet polyurethane.
  • FIG. 3 A suggested mechanism for the collapse of microcapsules immersed in wet coatings is illustrated in FIG. 3 .
  • the pressure inside the microcapsule 201 from the compound or compounds contained therein counteracts the pressure from the wet coating (not shown separately) surrounding the microcapsule, thus maintaining microcapsule structural integrity.
  • Diffusion of core material as at B from inside the microcapsule 201 through its shell to the outside creates empty space 301 in the cavity of the microcapsule 201 , disrupting the pressure balance aforementioned.
  • substantial compound (core material) diffuses from a microcapsule 201 , as at C the microcapsule collapses 202 inward.
  • Small gelatin microcapsules 101 are not appropriate for wet coatings if immersed therein more than two (2) weeks. The reason for this poor stability may be due to attack of the gelatin by the solvents either internal to the shell, i.e., the core material, external to the shell, i.e., the wet coating, or both. Further, even UF microcapsules 201 immersed in wet coatings have, a relatively short shelf life, thus, in a preferred embodiment of the present invention, microcapsules 201 should be mixed into the wet coating at the time of application.
  • UF microcapsules 201 greater than about 63 ⁇ in diameter should be employed for the containment and delivery of the self-healing compounds (core material). Larger microcapsules 201 contain and deliver more core material once ruptured than the smaller microcapsules 101 . Also, there is a higher probability of rupturing a small number of large microcapsules 201 than rupturing a large number of small microcapsules 101 to deliver the same volume of core material.
  • volume in terms of d is 4/3 ⁇ (d/2) 3 or 1 ⁇ 6 ⁇ d 3 .
  • the volume of the spheres of FIG. 5B i.e., 1 ⁇ 3 the diameter of the large sphere of FIG. 5A , is given by 1 ⁇ 6 ⁇ (d/3) 3 or 1 ⁇ 6 ⁇ d 3 /27.
  • a perpendicular cutting plane of the same area (150 ⁇ 150 ⁇ ) as used in FIG. 5A will completely sever only nine (9) of the small microcapsules 521 .
  • microcapsules 501 will deliver microcapsule contents over an optimum area of compromise, thus assuring the opportunity of assuring a better seal along the perimeter of the compromise.
  • Microcapsules much greater than 150 microns in diameter are too large for many coating applications, as conventional paint films (primers+topcoats) are only eight (8) mils (200 ⁇ ) in thickness for both coats. Thus, microcapsules of 63-150 microns are recommended for typical applications of these types of coatings.
  • Microcapsules incorporated in coatings to be applied to steel substrates for corrosion testing preferably have core compositions with corrosion inhibiting “healants,” such as film-forming compounds containing polybutene or phenolics, and one or more pre-specified corrosion inhibiting compounds.
  • core material contains certain diluents that facilitate flow of the film-forming compounds upon rupture of the microcapsule.
  • Primers and topcoats may be chosen from among acrylics and epoxy formulations. In all cases, the primers and topcoats and the core materials must be selected to not degrade the preferred UF shell material used in formulating the microcapsule.
  • Coatings used in testing preferred embodiments of the present invention include a paint primer, Dexter 1 OPW20-4 Water Reducible Epoxy Primer, Dexter-Hysol Company, and a paint topcoat, Sherwin-Williams Dura-Pox Water-based Epoxy Finish, Sherwin-Williams Paint Company.
  • Samples were applied to steel panels (not shown separately except for partial representation in the micrographs of FIGS. 1 , 2 and 4 ) obtained from Q-Panel Laboratory Products, Cleveland, Ohio 44145. They are described as Type R39 and conform to ASTM Specification A366, D609-Type 1. The panels are 3′′ ⁇ 9′′ ⁇ 0.032′′.
  • Microcapsules are added to the mixed primer at 25% weight based upon the dry solids contained in the primer. Microcapsules are added directly to the primer in small portions with slow mixing until all of the microcapsules appear to be wetted.
  • the primer and topcoat are applied using a drawdown bar. The samples are dried for one to two days after the primer is applied and for two (2) weeks after the topcoat is applied.
  • Microcapsules selected for evaluation are UF shells of 63-150 micron diameter with core materials selected from the following candidates: phenolic varnish; a long chain polyester diluent; Iso decyl diphenyl phosphate, commercially available as SANTICIZ ⁇ R® 148, Solutia, Inc., St. Louis, Mo.; a second carrier/diluent, modified partially hydrogenated terphenol, commercially available as THERMINOL® 66, Solutia, Inc., St.
  • ASTM D 5894 testing combines the environmental effects of salt spray and UV light, simulating exposure to field conditions.
  • EIS electrochemical impedance spectroscopy
  • FIG. 4 depicts the rupture pattern 401 of UF microcapsules upon inducing a crack in the applied coating while FIG. 4B depicts the rupture “line” 402 of UF microcapsules upon scribing the applied coating.
  • results for the “control” and the three (3) self-healing coatings, as formulated with microcapsules of three different compositions, are shown in FIG. 6 .
  • the amount of undercutting for each panel is determined by taking the mean maximum of the coating loss extending between the top and bottom of each of two scribe marks, according to the procedure recommended by ASTM D 1654. These results are shown as a plot of mean undercutting (in mm) for all microcapsules in each sample set by microcapsule type for the four sample types (three microcapsule formulations A, C, D and a control or None).
  • microcapsules with “self-healing” compounds and corrosion inhibitors significantly reduces undercutting at the scribe, compared to the control coatings containing no microcapsules.
  • the undercutting was reduced from a mean value of 2.12 mm for the control to a mean value of 0.39 mm for the coatings containing the “C” microcapsules.
  • Performance of epoxy-based primers is enhanced by the addition of appropriately fabricated microcapsules. Burst microcapsules counteract the effects of ultraviolet light and salt spray exposure, releasing “healing compounds” when damaged, e.g., by scribing.
  • the core material in the microcapsules fulfilled expectations.
  • the phenolic varnish acted as a film-former to seal the edges of the damaged coating.
  • the diluents functioned as a low viscosity carrier/diluent for the other components.
  • the camphor, and the two anti-corrosion agents, A and B functioned as viable corrosion control agents to provide additional corrosion protection over at least part of the scribed region.
  • Electrochemical impedance spectroscopy is performed on the scribed area of one of the coating system samples containing the “C” microcapsules in the coating, and on the scribed area of one of the control samples after both were subjected to the ASTM D 5894 test.
  • the EIS results are presented in FIG. 7 as Log Impedance Modulus ( ⁇ ) vs. Log Frequency (Hz), and in FIG. 8 , as Phase Angle (deg) vs. Log Frequency (Hz), respectively. Over a frequency range of 100 KHz to 0.1 Hz, the impedance moduli of the scribed areas of either the control coating or the “C” microcapsule coating did not change significantly.
  • the impedance modulus of the scribed area of the sample containing the “C” microcapsules is about 16 times greater than the impedance modulus of the scribed area of the coating with no microcapsules. This is an objective indicator of the “C” microcapsules having sealed the substrate, preventing further growth of the scribed area.
  • the phase angles for both coatings display slightly negative values, with a suggestion of less on-going corrosion of the “C” microcapsule sample.
  • the phase angles for coatings with the “C” microcapsules display a slightly more capacitive behavior, as would be expected for an uncompromised coating.
  • the EIS results are consistent with the undercutting measurements previously described.

Abstract

A self-healing coating, incorporating medium-sized microcapsules filled with a liquid formulation, repairs itself upon physical compromise. In one embodiment, a commercial primer is mixed with these microcapsules and applied. After the coating has cured, any physical compromise of the cured coating results in the microcapsules bursting to release the liquid, in turn filling and sealing the compromised volume of the coating. In applications where a product is used to provide corrosion protection, the liquid contains anti-corrosion material as well as suitable diluents and film-forming compounds. In a preferred embodiment, the microcapsules are provided separately to be mixed with commercial products during preparation for application of the coating. For example, if a paint formulation is known a priori, tailored microcapsules packaged separately from the paint and designed for use with the paint formulation, are wet mixed into the paint during preparation for application.

Description

    RELATED APPLICATIONS
  • This application claims the benefit under 35 U.S.C § 120 of prior co-pending U.S. patent application Ser. No. 10/377,642, Self-Healing Coating and Microcapsules to Make Same, by Sarangapani et al., filed Mar. 4, 2003, and incorporated herein by reference.
  • STATEMENT OF GOVERNMENT INTEREST
  • Under paragraph 1(a) of Executive Order 10096, the conditions under which this invention was made entitle the Government of the United States, as represented by the Secretary of the Army, to the entire right, title and interest therein of any patent granted thereon by the United States. This patent and related ones are available for licensing. Contact Bea Shahin at 217 373-7234 or Phillip Stewart at 601 634-4113.
  • FIELD OF THE INVENTION
  • The present invention relates generally to coatings, in particular coatings that have been modified to provide a self-healing characteristic.
  • BACKGROUND
  • Much effort and resources are expended in ongoing corrosion control, even when an item has been coated initially to protect it. Abrasion, saltwater, high humidity, ultraviolet light, temperature gradients, and other deleterious environmental factors contribute to this, alone or in combination. To conserve corrosion control resources, it would be beneficial to use not only a “tough” initial protective coating, but also a coating that, when compromised, “heals” itself.
  • There have been efforts to effect a self-repairing capability in various materials, notably shaped articles that may be made of materials with a weakness in one or more orientations, such as cementitious materials having inherently poor tensile strength. U.S. Pat. No. 5,575,841, Cementitious Materials, to Dry, Nov. 19, 1996, and U.S. Pat. Nos. 5,660,624 (Aug. 26, 1997), 5,989,334 (Nov. 23, 1999), and 6,261,360 B1 (Jul. 17, 2001), each entitled Self-Repairing Reinforced Matrix Materials, all to Dry, detail a method of incorporating hollow fibers in “pourable” material to effect a self-repairing function. These inventions employ selectively releasable compounds within the hollow fiber. Because of the size of the fibers, these patents are unsuitable for repair upon a smooth surface.
  • Microcapsules contain minute amounts of product for specialized delivery, often size, time or location critical. They may be obtained in diameters of less than 250 microns (μ) and have been used in a variety of applications, from the pharmaceutical industry (delivery of drugs) to the textile industry (providing protective wear for HAZMAT workers). One example is U.S. Pat. No. 6,060,152, Fabric with Microencapsulated Breach Indication Coating, to Murchie, May 9, 2000. The '152 patent describes a membrane incorporating a number of different microcapsules that alert to even the smallest compromise of the fabric comprising a protective suit such as may be worn by a HAZMAT worker or health professional.
  • Very recent work to improve coatings by the addition of additives involves only improving the application of the coating to a substrate, not the ability of the coating to “repair” itself upon its compromise. One such example is U.S. Pat. No. 6,746,522 B2, High Molecular Weight Polymer Additive for Coating and Protective Products, to Trippe et al., Jun. 8, 2004. The '522 patent details the advantages of adding small amounts of an ultrahigh molecular weight polymer, such as polyisobutylene, to enhance coating properties of a solvent. Once, a nick compromises the coating or abrasion, however, another separately applied application is required to protect the substrate.
  • Another concern in using microcapsules with solvents is the timing of delivery of the encapsulated compound. Prior patents have avoided this timing problem by mixing the microcapsules with dry powder coatings such as are used in “powder coating” applications involving elevated temperatures. U.S. Pat. No. 6,075,072, Latent Coating for Metal Surface Repair, to Guilbert et al., Jun. 13, 2000, details a self-repairing compound suitable for use in powder coating. By adding microcapsules of sufficiently small size, i.e., 10-40μ, to a dry powder form of protective coating, the resultant “self-repairing” coating is able to be powder coated upon metal substrates at suitable elevated temperatures that melt the coating to a homogenous continuous surface of approximately 200μ thickness. The microcapsules used with the '072 patent are mixed in the dry state to prevent short-term degradation of the shells by liquid solvents.
  • Unless appropriate materials are used to fabricate the microcapsule and its contents, it may “deploy” before the coating is applied or, upon application, spontaneously deploy improperly, i.e., without a physical compromise of the coating such as abrasion or nicking. Further, unless the microcapsule is compatible with both its contents (the encapsulated repair compound) and its surrounds (the solvent), the “application” life of the resultant mixed product may be less than desirable. These constraints have been addressed in the present invention.
  • SUMMARY
  • In a preferred embodiment of the present invention, urea formaldehyde microcapsules, approximately 60-150 microns (μ) in diameter and containing corrosion inhibitors and several types of film forming compounds, or “healants,” are mixed with commercially available coatings. When the applied modified coating is damaged, e.g., by abrasion through the coating to the substrate on which it is applied, the microcapsules burst, releasing the film forming and corrosion inhibiting compounds. This initiates a self-healing process, i.e., the damaged area of the substrate is covered and repaired, inhibiting corrosion. Steel substrates coated with these modified coatings, or “self-healing systems,” were scribed and laboratory tested according to ASTM D 5894, i.e., alternately exposing them to salt spray and ultraviolet (UV) light. ASTM D-5894, Standard Practice for Cyclic Salt Fog/UV Exposure of Painted Metal, (Alternating Exposures in a Fog/Dry Cabinet and a UV Condensation Cabinet), American Society for Testing Materials, West Conshohocken, Pa. The coated test specimens were evaluated with respect to undercutting at the scribe in accordance with ASTM D 1654. ASTM D 1654, Standard Practice for Cyclic Salt Fog/UV Exposure of Painted Metal, (Alternating Exposures in a Fog/Dry Cabinet and a UV Condensation Cabinet), American Society for Testing Materials, West Conshohocken, Pa. The undercutting was reduced from 2.12 mm to 0.46 mm at the scribe when employing microcapsules containing phenolic varnish, a long chain polyester diluent, a second carrier/diluent based on high molecular weight hydrocarbons and a corrosion inhibitor. Electrochemical impedance spectroscopy (EIS) tests showed that the incorporation of self-healing microcapsules resulted in significantly higher impedances for damaged “microcapsule coatings” than for the same coatings containing no microcapsules.
  • Thus, in general, a self-healing coating is provided that, after application and curing upon a substrate, self heals upon its physical compromise. It comprises one or more solvents, one or more solids and microcapsules containing a repair material that may comprise one or more substances. The shell of the microcapsule is resistant to degradation from within by the repair substances. Prior to application of the self-healing coating and after addition of the microcapsules to a solvent/solid mixture, the microcapsules are resistant to short term degradation of the exterior shell by either the solvents or the solids. The microcapsules burst upon physical compromise of the resultant applied and cured coating, releasing the repair substances to seal a volume (void) within the coating cause by the physical compromise. Spherical microcapsules produce a most efficient delivery volume and are preferred. However, other shapes, such as filaments, may be used also, with a concomitant loss of efficiency. In addition to traditional paints, the microcapsules may be used with or deliver greases, lubricants, varnishes, lacquers, shellacs, polyurethanes, waxes, polishes, fabric treatments, waterproofing compounds, liquid roofing coatings, oils, and similar compounds.
  • The combination of one or more solvents and one or more solids may comprise a protective coating that would serve the purpose of protecting a substrate but not have the self-healing properties of the present invention. This protective coating may be one of a number of commercially available products, to include primer paints, topcoat paints, “one coat” or “self-priming” paints, varnishes, lacquers, polyurethane finishes, shellacs, waxes, polishes, “one step” finishing preparations for wood, metal, or synthetic materials, and combinations thereof. The paint primers may be: polyurethanes, oil-based enamels, enamel undercoater, latex acrylics, acrylic formulations and epoxy formulations. Further, topcoat and self-priming paints may be: polyurethanes, oil-based enamels, enamels, latex acrylics, acrylic formulations and epoxy formulations.
  • Any of the coatings may serve as a corrosion inhibitor through the addition of suitable corrosion inhibitors or the coatings may be merely decorative.
  • The shell of the microcapsule may be a sphere with an outer diameter preferably within the approximate range of 50 to 200μ. More preferably, the shell may be a sphere with an outer diameter greater than approximately 63μ. Most preferably, the shell is a sphere with an outer diameter of approximately 150μ.
  • The shell of the microcapsule may comprise either gelatin or, more preferably, urea formaldehyde (UF).
  • The repair substances may be a combination of film-forming compounds and corrosion inhibiting compounds. The film-forming compounds may be any of: polybutenes, phenolics, phenolic varnishes, long chain polyester diluents, carrier diluents, and combinations thereof. The corrosion inhibiting compounds may be any of: camphor, alkylammonium salt in xylene, Ciba IRGACOR® 153 (hereafter also anti-corrosion agent A), polyamine fatty acid in salt in ethanol, Ciba IRGACOR® 287 (hereafter also anti-corrosion agent B), and combinations thereof.
  • The microcapsules are added prior to application as a pre-specified percentage of the dry weight of the solids in the base coating at a pre-specified time prior to application of the self-healing coating. Preferably, the pre-specified percentage lies in the approximate range of 10 to 40% and the microcapsules are added within fourteen (14) days of application. Most preferably, the pre-specified percentage is approximately 25% and the microcapsules are added when preparing the coating for application.
  • Also provided is the microcapsule suitable for adding to available protective coatings to facilitate self-healing thereof after application and curing. In general, this microcapsule comprises a repair substance and a shell enclosing a volume containing the repair substance. Upon application of the protective coating to a substrate and curing of the coating thereon, physical damage to the resultant coating ruptures the shell of the microcapsules in the vicinity of the rupture and deploys the repair substance into a volume (void) within the coating caused by the physical damage.
  • The shell of the microcapsule may be a sphere with an outer diameter preferably within the approximate range of 50 to 200μ. More preferably, the shell has an outer diameter greater than approximately 63μ. Most preferably, the shell has an outer diameter of approximately 150μ.
  • The shell of the microcapsule may be gelatin, or preferably urea formaldehyde (UF). The repair substance contained therein may comprise film-forming compounds and corrosion inhibiting compounds.
  • The film-forming compounds may be any of: polybutenes, phenolics, phenolic varnishes, and combinations thereof. The diluents may be any of: long chain polyester diluents, carrier diluents, and combinations thereof. The corrosion inhibiting compounds may be any of: camphor; alkylammonium salt in xylene, commercially available as Ciba IRGACOR® 153 (anti-corrosion agent A); polyamine fatty acid in salt in ethanol, commercially available as Ciba IRGACOR® 287 (anti-corrosion agent B); and combinations thereof.
  • Also provided is a method for making a self-healing coating. It comprises: (a) providing a non-self healing coating; (b) providing microcapsules filled with a repair substance compatible with the non-self healing coating; and (c) mixing the microcapsules into the non-self healing coating such that the microcapsules are fully wetted and interspersed evenly throughout the non-self healing coating.
  • Further provided is a method for producing a self-healing coating upon a substrate. It comprises: (a) providing a non-self healing coating; (b) providing microcapsules filled with a repair substance compatible with the non-self healing coating; (c) mixing the microcapsules into the non-self healing coating such that the microcapsules are fully wetted and interspersed evenly throughout the non-self healing coating; (d) applying the self-healing coating to the substrate by any of a number of means selected from the group consisting of: brushing, rolling, spraying, and combinations thereof; and (e) permitting the applied self-healing coating to cure prior to use of the substrate.
  • Advantages of preferred embodiments of the present invention include:
  • reduced need for maintenance and renewal of applied protective coatings;
  • reduced maintenance costs;
  • increased intervals between required inspections;
  • reduced life cycle costs;
  • improved appearance of the substrate over its design life;
  • increased service life of an item protected with the self-healing coating; and
  • increased mean time between failure (MTBF).
  • Further advantages of the present invention will be apparent from the description below with reference to the accompanying drawings, in which like numbers indicate like elements.
  • BRIEF DESCRIPTION OF THE DRAWINGS
  • FIG. 1A is a micrograph typical of small gelatin microcapsules (<63μ diameter) as collapsed when immersed in wet polyurethane when investigated for possible use in the present invention.
  • FIG. 1B is a micrograph typical of medium gelatin microcapsules (63-150μ diameter) after two (2) hours immersion in wet polyurethane when investigated for possible use in the present invention.
  • FIG. 2A is a micrograph typical of large urea-formaldehyde (UF) microcapsules (>150μ diameter) after two (2) weeks immersion in wet polyurethane when investigated for possible use in the present invention.
  • FIG. 2B is a micrograph typical of large urea-formaldehyde (UF) microcapsules (>150μ diameter) deteriorating after four (4) weeks immersion in wet polyurethane when investigated for possible use in the present invention.
  • FIG. 3 depicts a suggested mechanism for the collapse of microcapsules in wet coatings.
  • FIG. 4A is a micrograph showing the effect of burst UF microcapsules incorporated in applied coatings of the present invention in which a crack is induced in the coating.
  • FIG. 4B is a micrograph showing the effect of burst UF microcapsules incorporated in applied coatings of the present invention in which the coating has been scribed.
  • FIG. 5A depicts a cross section through a cube containing a single large microcapsule that may be used in a preferred embodiment of the present invention.
  • FIG. 5B depicts a cross section through the cube of FIG. 5A with a superimposed symmetric array of nine small microcapsules that fit in the same cube containing the large microcapsule of FIG. 5A.
  • FIG. 6 details the test results for the control and the three (3) self-healing coatings that may be employed as preferred embodiments of the present invention.
  • FIG. 7 depicts the relationship between impedance and frequency for both a control sample and a preferred embodiment of the present invention using data taken with Electrochemical Impedance Spectroscopy (EIS).
  • FIG. 8 depicts the relationship between phase angle and frequency for both a control sample and a preferred embodiment of the present invention using data taken with EIS.
  • DETAILED DESCRIPTION
  • A preferred embodiment of the present invention provides a “self-healing” coating system that may be used for corrosion protection, such as on outdoor steel cabinet enclosures for electrical equipment. Microcapsules in the form of microscopic spheres with a diameter of 50-200μ, and more preferably of 60-150μ diameter, are used to encapsulate “coating repairing” compounds as a means of effecting self-healing of the applied coating thus derived. These microcapsules are fabricated for optimum dispersal into various coating formulations, e.g., paint, enabling release of the coating repairing or “self-healing” compounds. These compounds may comprise, at least in part, corrosion-inhibiting constituents. Thus, when the applied coating is mechanically ruptured such as may occur upon damage by impact or abrasion, these compounds are “deployed.” Corrosion-inhibiting microcapsules may be used in coating systems to minimize damage caused by scratches or abrasions by releasing specially formulated chemicals that flow into the damaged areas forming thin films of corrosion protection.
  • For paint systems, self-healing coatings are fabricated by adding microcapsules containing at least one “self-healing” compound to commercially available paint primers. Paint primers may include those paints commercially termed “one coat” or “self-priming.” The microcapsules release the self-healing compound or compounds, most commonly as liquids, when the coating system is damaged. Urea formaldehyde (UF) microcapsules of 50-150μ in diameter have been added to primers with an applied thickness of 0.1 mm (0.004″) to increase the coating service life by “self-healing” damaged areas. Verification of performance was conducted by accelerated corrosion testing on conventional coating systems using ASTM D 5894 and Electrochemical Impedance Spectroscopy (EIS). M. Kendig and J. Scully, Basic Aspects of Electrochemical Impedance Applications for the Life Prediction of Organic Coatings on Metals, Corrosion, Vol. 46, No. 1, pp. 22-29, 1990. H. Hack and J. Scully, Defect Area Determination of Organic Coated Steels in Seawater Using the Breakpoint Frequency Method, J. Electrochem. Soc., Vol. 138, No. 1, pp. 33-40, 1991.
  • One of the primary concerns in using microcapsules in coatings that contain solvents is the maintenance of structural integrity of the microcapsule until application of the coating and evaporation of the solvent or solvents. A laboratory study was undertaken to determine the stability of both urea formaldehyde (UF) and gelatin as shell materials as well as the propensity of the microcapsules to release the “self-healing” compounds only when the applied coating is physically damaged. The gelatin and UF capsules are filled with red dye as a tracer to facilitate evaluation.
  • Achieving timely and appropriate rupturing of microcapsules to be incorporated in applied coatings is crucial to developing and commercializing “self-healing” coatings. “Timely and appropriate rupturing” occurs, for example, when the applied coating is damaged physically or if cracks develop in the applied coating. Microcapsules may exhibit at least two major “improper rupturing” modes; viz., rupturing before the coating is applied to a surface and spontaneous rupturing on the surface of applied coatings prior to cracking or physical damage.
  • To determine the stability of the microcapsules in various coating formulations, samples of each are bottled. Samples are extracted from each bottle and placed on glass slides. Initial optical micrographs of each are taken. After initial sampling, each bottle is tightly sealed. Optical micrographs of each sample are taken weekly over a period of four (4) weeks, and deterioration (if any) as a function of time is noted. A listing of the types and quantities of tested microcapsules, designated as: small (<63μ), medium (63-150μ), and large (>150μ), is shown in Table 1.
  • TABLE 1
    Wet Coatings Investigated for Stability of Microcapsules
    SIZE OF
    SAMPLE TYPE OF PAINT AND CAPSULES AND
    NUMBER AMOUNT (grams) AMOUNT (grams)
    1 Polyurethane 35 Medium 0.6
    2 Polyurethane 100 Medium 0.3
    3 Polyurethane 100 Large 0.6
    4 Polyurethane 100 Small 0.6
    5 Oil-based enamel (flat white) 100 Medium 0.6
    6 Acrylic primer (latex) 100 Medium 0.6
    7 Interior enamel (latex acrylic) 100 Medium 0.6
    8 Enamel under coater 100 Medium 0.6
    9 Acrylic primer (latex) 50 Small 0.6
  • Refer to the micrographs of FIG. 1. Small gelatin microcapsules 101 (diameters less than 63μ) failed to maintain structural integrity and self ruptured in polyurethane and other coatings in a few days. A micrograph typical of collapsed small gelatin microcapsules 101 is shown in FIG. 1A. As depicted in FIG. 1B after two hours immersion in polyurethane, medium (63-150μ) gelatin microcapsules 102 maintain integrity somewhat longer than a few days. As shown in the micrograph of FIG. 2A, large UF microcapsules 201 (diameter greater than 150μ) maintained integrity for at least two (2) weeks. However, as shown in the micrograph of FIG. 2B, even the large UF microcapsules 201 began to collapse 202 and lose core material after four (4) weeks immersion in wet polyurethane.
  • A suggested mechanism for the collapse of microcapsules immersed in wet coatings is illustrated in FIG. 3. Upon initial introduction of microcapsules to the wet coating as shown at A, the pressure inside the microcapsule 201 from the compound or compounds contained therein counteracts the pressure from the wet coating (not shown separately) surrounding the microcapsule, thus maintaining microcapsule structural integrity. Diffusion of core material as at B (from inside the microcapsule 201 through its shell to the outside) creates empty space 301 in the cavity of the microcapsule 201, disrupting the pressure balance aforementioned. After substantial compound (core material) diffuses from a microcapsule 201, as at C the microcapsule collapses 202 inward.
  • Small gelatin microcapsules 101 are not appropriate for wet coatings if immersed therein more than two (2) weeks. The reason for this poor stability may be due to attack of the gelatin by the solvents either internal to the shell, i.e., the core material, external to the shell, i.e., the wet coating, or both. Further, even UF microcapsules 201 immersed in wet coatings have, a relatively short shelf life, thus, in a preferred embodiment of the present invention, microcapsules 201 should be mixed into the wet coating at the time of application.
  • For best results, UF microcapsules 201 greater than about 63μ in diameter should be employed for the containment and delivery of the self-healing compounds (core material). Larger microcapsules 201 contain and deliver more core material once ruptured than the smaller microcapsules 101. Also, there is a higher probability of rupturing a small number of large microcapsules 201 than rupturing a large number of small microcapsules 101 to deliver the same volume of core material.
  • Refer to FIG. 5. Consider, for example, a simple cube 500, 520 of dimension, d, on a side with a distribution of one or more microcapsules therein. The volume of a sphere is 4/3 πr3, where r=d/2. Thus, volume in terms of d is 4/3π(d/2)3 or ⅙πd3. If as shown by comparing the microcapsules (spheres) in FIG. 5A to those in FIG. 5B, the volume of the spheres of FIG. 5B, i.e., ⅓ the diameter of the large sphere of FIG. 5A, is given by ⅙π(d/3)3 or ⅙πd3/27. Thus, assuming “perfect packing” of 27 small spheres of diameter d/3 in the same cube of dimension d, the same amount of core material is available within the cube. “Perfect packing” of the cube may be impossible to achieve but does serve to illustrate the point theoretically. As an example, for a large single microcapsule 501 just fitting the cube 510 of dimension d, its diameter d may be 150μ. A perpendicular cutting plane of 150×150μ will completely sever this single large microcapsule 501, delivering a volume of 1.8×106μ3. As depicted only in cross section 520 in FIG. 5B, the equivalent volume of the same cube 510 may be filled by 27 smaller microcapsules 521, each of diameter, ds=50μ, where ds=d/3. However, a perpendicular cutting plane of the same area (150×150μ) as used in FIG. 5A will completely sever only nine (9) of the small microcapsules 521. This yields a combined volume of 0.6×106μ3 of core material, only ⅓ of the single large microcapsule 501 of FIG. 5A. Thus, even under the assumption of optimal packing for the small microcapsules 521, the larger microcapsules 501 will deliver microcapsule contents over an optimum area of compromise, thus assuring the opportunity of assuring a better seal along the perimeter of the compromise. Microcapsules much greater than 150 microns in diameter are too large for many coating applications, as conventional paint films (primers+topcoats) are only eight (8) mils (200μ) in thickness for both coats. Thus, microcapsules of 63-150 microns are recommended for typical applications of these types of coatings.
  • Microcapsules incorporated in coatings to be applied to steel substrates for corrosion testing preferably have core compositions with corrosion inhibiting “healants,” such as film-forming compounds containing polybutene or phenolics, and one or more pre-specified corrosion inhibiting compounds. As well, core material contains certain diluents that facilitate flow of the film-forming compounds upon rupture of the microcapsule. Primers and topcoats may be chosen from among acrylics and epoxy formulations. In all cases, the primers and topcoats and the core materials must be selected to not degrade the preferred UF shell material used in formulating the microcapsule.
  • Coatings used in testing preferred embodiments of the present invention include a paint primer, Dexter 1 OPW20-4 Water Reducible Epoxy Primer, Dexter-Hysol Company, and a paint topcoat, Sherwin-Williams Dura-Pox Water-based Epoxy Finish, Sherwin-Williams Paint Company. Samples were applied to steel panels (not shown separately except for partial representation in the micrographs of FIGS. 1, 2 and 4) obtained from Q-Panel Laboratory Products, Cleveland, Ohio 44145. They are described as Type R39 and conform to ASTM Specification A366, D609-Type 1. The panels are 3″×9″×0.032″.
  • Microcapsules are added to the mixed primer at 25% weight based upon the dry solids contained in the primer. Microcapsules are added directly to the primer in small portions with slow mixing until all of the microcapsules appear to be wetted. The primer and topcoat are applied using a drawdown bar. The samples are dried for one to two days after the primer is applied and for two (2) weeks after the topcoat is applied.
  • Microcapsules selected for evaluation are UF shells of 63-150 micron diameter with core materials selected from the following candidates: phenolic varnish; a long chain polyester diluent; Iso decyl diphenyl phosphate, commercially available as SANTICIZÈR® 148, Solutia, Inc., St. Louis, Mo.; a second carrier/diluent, modified partially hydrogenated terphenol, commercially available as THERMINOL® 66, Solutia, Inc., St. Louis, Mo.; and either camphor or a corrosion inhibitor in either of two forms as alkylammonium salt in xylene, commercially available as Ciba IRGACOR® 153 or polyamine fatty acid in salt in ethanol, commercially available as Ciba IRGACOR® 287, Ciba Geigy Company. The only difference in the three microcapsule core materials that were tested is in the addition of one extra component in each. The extra component in the microcapsules designated “A” is “anti-corrosion agent A”; that designated “C” is “anti-corrosion agent B” and that designated “D” is camphor.
  • Four (4) sets of samples of three (3) panels each are tested. The edges and backs of all coated steel panel samples are sealed using a coal tar epoxy composition. The first set is the control, having no microcapsules in the coating. Three sets are formulated similarly to the control except for incorporating microcapsules in the primer at 25% of dry weight of solids in the primer. After allowing the samples to cure fully, two scribe marks are made on each sample panel per ASTM D 1654.
  • Accelerated corrosion testing for 2016 hours is accomplished under ASTM D 5894. ASTM D5894 testing combines the environmental effects of salt spray and UV light, simulating exposure to field conditions. In addition, electrochemical impedance spectroscopy (EIS) evaluations were performed on some samples subsequent to the ASTM D 5894 tests in order to determine the relative degree of coating degradation at the scribed area.
  • Representative self-healing “deployments” are shown in FIG. 4. FIG. 4A depicts the rupture pattern 401 of UF microcapsules upon inducing a crack in the applied coating while FIG. 4B depicts the rupture “line” 402 of UF microcapsules upon scribing the applied coating.
  • Results for the “control” and the three (3) self-healing coatings, as formulated with microcapsules of three different compositions, are shown in FIG. 6. The amount of undercutting for each panel is determined by taking the mean maximum of the coating loss extending between the top and bottom of each of two scribe marks, according to the procedure recommended by ASTM D 1654. These results are shown as a plot of mean undercutting (in mm) for all microcapsules in each sample set by microcapsule type for the four sample types (three microcapsule formulations A, C, D and a control or None). This clearly shows that addition of microcapsules with “self-healing” compounds and corrosion inhibitors significantly reduces undercutting at the scribe, compared to the control coatings containing no microcapsules. For example, the undercutting was reduced from a mean value of 2.12 mm for the control to a mean value of 0.39 mm for the coatings containing the “C” microcapsules.
  • Further, differences were noted among the undercutting results for the three separate microcapsule formulations. The coatings with the “C” microcapsules (mean undercutting of 0.39 mm) that contained Anti-Corrosion Agent “B”, performed only slightly better than the “D” microcapsules, containing the camphor (mean undercutting of 0.46 mm). However, coatings with either the “C” or “D” microcapsules performed significantly better than coatings with the “A” microcapsules, containing Anti-Corrosion Agent “A” (mean undercutting of 0.75 mm). Undercutting measurements taken in this way provide a measure of the relative ability of the coating system to adhere at the scribe where corrosion is taking place, and to resist underfilm corrosion.
  • Performance of epoxy-based primers is enhanced by the addition of appropriately fabricated microcapsules. Burst microcapsules counteract the effects of ultraviolet light and salt spray exposure, releasing “healing compounds” when damaged, e.g., by scribing. The core material in the microcapsules fulfilled expectations. The phenolic varnish acted as a film-former to seal the edges of the damaged coating. The diluents functioned as a low viscosity carrier/diluent for the other components. The camphor, and the two anti-corrosion agents, A and B, functioned as viable corrosion control agents to provide additional corrosion protection over at least part of the scribed region.
  • Refer to FIGS. 7 and 8. Electrochemical impedance spectroscopy (EIS) is performed on the scribed area of one of the coating system samples containing the “C” microcapsules in the coating, and on the scribed area of one of the control samples after both were subjected to the ASTM D 5894 test. The EIS results are presented in FIG. 7 as Log Impedance Modulus (Ω) vs. Log Frequency (Hz), and in FIG. 8, as Phase Angle (deg) vs. Log Frequency (Hz), respectively. Over a frequency range of 100 KHz to 0.1 Hz, the impedance moduli of the scribed areas of either the control coating or the “C” microcapsule coating did not change significantly. Note however, that the impedance modulus of the scribed area of the sample containing the “C” microcapsules is about 16 times greater than the impedance modulus of the scribed area of the coating with no microcapsules. This is an objective indicator of the “C” microcapsules having sealed the substrate, preventing further growth of the scribed area. The phase angles for both coatings display slightly negative values, with a suggestion of less on-going corrosion of the “C” microcapsule sample. The phase angles for coatings with the “C” microcapsules display a slightly more capacitive behavior, as would be expected for an uncompromised coating. Thus, the EIS results are consistent with the undercutting measurements previously described.
  • While the invention has been described in terms of its preferred embodiments, those skilled in the art will recognize that the invention may be practiced with modifications within the spirit and scope of the appended claims. For example, although the system is described in specific examples for paints, it is amenable for use with other coatings that one desires to prolong in an uncompromised state or to retain an original capacity for protection, regardless of outward appearance. These coatings may include merely decorative coatings as well as the aforementioned corrosion inhibiting coatings. Thus, it is intended that all matter contained in the foregoing description or shown in the accompanying drawings shall be interpreted as illustrative rather than limiting, and the invention should be defined only in accordance with the following claims and their equivalents.

Claims (30)

1. A self-healing coating that repairs itself upon physical compromise of an application of said self-healing coating that was cured at ambient temperature, comprising:
at least one liquid COTS coating containing at least some solids; and
medium-sized microcapsules, having a shell defining a volume of a sphere with an average outer diameter between 80 and approximately 150 microns, said volume containing at least one repair substance, said medium-sized microcapsules wet mixed into said liquid COTS coating just prior to application of said self-healing coating,
wherein said shell is resistant to degradation by said repair substance; and
wherein prior to application of said self-healing coating and after addition of said microcapsules to said liquid COTS coating, said microcapsules are resistant to short term degradation by said liquid COTS coating; and
wherein said microcapsules in the area of a physical compromise of said applied and cured self-healing coating burst, releasing said at least one repair substance to fill and seal the compromised volume within said self-healing coating.
2. The self-healing coating of claim 1 in which said at least one liquid COTS coating comprises a protective coating.
3. The self-healing coating of claim 2 in which said protective coating is a paint.
4. The self-healing coating of claim 3 in which said paint is a primer selected from the group consisting of: polyurethanes, oil-based enamels, enamel undercoater, latex acrylics, acrylic formulations and epoxy formulations.
5. The self-healing coating of claim 3 in which said paint is a topcoat selected from the group consisting of: polyurethanes, oil-based enamels, enamels, latex acrylics, acrylic formulations and epoxy formulations.
6. The self-healing coating of claim 3 in which said paint is a self-priming paint selected from the group consisting of: polyurethanes, oil-based enamels, enamels, latex acrylics, acrylic formulations and epoxy formulations.
7. The self-healing coating of claim 1 in which the combination of said liquid COTS coating and said microcapsules comprises a corrosion inhibiting coating.
8. The self-healing coating of claim 1 in which the combination of said liquid COTS coating and said microcapsules comprises a decorative coating.
9. The self-healing coating of claim 1 in which the average outer diameter of said microcapsule is approximately 100 to 150 microns.
10. The self-healing coating of claim 1 in which the average outer diameter of said microcapsule is approximately 150 microns.
11. The self-healing coating of claim 1 in which said shell comprises urea formaldehyde (UF).
12. The self-healing coating of claim 1 in which said shell comprises gelatin.
13. The self-healing coating of claim 1 in which said repair substance comprises:
film-forming compounds;
diluents; and
corrosion inhibiting compounds.
14. The self-healing coating of claim 13 in which said film-forming compounds are selected from the group consisting of polybutene, phenolics, phenolic varnishes, and combinations thereof.
15. The self-healing coating of claim 13 in which said diluents are selected from the group consisting of: long chain polyester diluents, carrier diluents, and combinations thereof.
16. The self-healing coating of claim 13 in which said corrosion inhibiting compounds are selected from the group consisting of: camphor, alkylammonium salt in xylene, polyamine fatty acid in salt in ethanol, and combinations thereof.
17. The self-healing coating of claim 1 in which said microcapsules are added as a pre-specified percentage of the dry weight of said solids to said liquid COTS coating at a pre-specified time prior to application of said self-healing coating.
18. The self-healing coating of claim 17 in which said pre-specified percentage lies in the approximate range of 10 to 40% and said pre-specified time is within the range of about immediately prior to application to about fourteen (14) days prior to application of said self-healing coating.
19. The self-healing coating of claim 18 in which said pre-specified percentage is approximately 25% and said pre-specified time is approximately concurrent with preparing said self-healing coating for application.
20. A microcapsule wet mixed into a liquid COTS coating to produce a self-healing coating cured at ambient temperature, said microcapsule comprising:
a repair substance; and
a shell enclosing a volume containing said repair substance, in which said shell is a sphere with an average outer diameter of approximately 80 to 150 microns,
whereupon application of said self-healing coating to a substrate and curing of said self-healing coating thereon, physical compromise of said self-healing coating results in rupture of said shells near said physical compromise and deployment of said repair substance to fill and seal the compromised volume within said self-healing coating.
22. The microcapsule of claim 20 in which said shell has an average outer diameter greater than 80 microns and less than 200 microns.
23. The microcapsule of claim 20 in which said shell has an average outer diameter of approximately 150 microns.
24. The microcapsule of claim 20 in which said shell comprises urea formaldehyde (UF).
25. The microcapsule of claim 20 in which said shell comprises gelatin.
26. The microcapsule of claim 20 in which said repair substance comprises:
film-forming compounds;
diluents; and
corrosion inhibiting compounds.
27. The microcapsule of claim 26 in which said film-forming compounds are selected from the group consisting of: polybutene, phenolics, phenolic varnishes, and combinations thereof.
28. The microcapsule of claim 26 in which said diluents are selected from the group consisting of: long chain polyester diluents, carrier diluents, and combinations thereof.
29. The microcapsule of claim 26 in which said corrosion inhibiting compounds are selected from the group consisting of camphor, alkylammonium salt in xylene, polyamine fatty acid in salt in ethanol, and combinations thereof.
30. A method for providing a liquid self-healing coating that repairs itself after application and curing, comprising:
providing a liquid non-self healing coating;
providing medium-sized microcapsules of an average diameter between approximately 80 and 150 microns filled with a repair substance compatible with said non-self healing coating; and
in preparation for applying said liquid self-healing coating, mixing said microcapsules into said liquid non-self healing coating such that said microcapsules are fully wetted and interspersed evenly throughout said liquid non-self healing coating.
31. A method for producing a self-healing coating upon a substrate, comprising:
providing a liquid non-self healing coating;
providing medium-sized microcapsules of an average diameter between approximately 80 and 150 microns filled with a repair substance compatible with said non-self healing coating;
in preparation for applying said self-healing coating, mixing said microcapsules into said liquid non-self healing coating such that said microcapsules are fully wetted and interspersed evenly throughout said liquid non-self healing coating thus producing a liquid self-healing coating;
applying said liquid self-healing coating to said substrate by any of a number of means selected from the group consisting of: brushing, rolling, spraying, and combinations thereof; and
permitting said applied liquid self-healing coating to cure prior to use of said substrate.
US11/789,811 2003-03-04 2007-02-22 Self-healing coating and microcapsules to make same Abandoned US20080152815A1 (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
US11/789,811 US20080152815A1 (en) 2003-03-04 2007-02-22 Self-healing coating and microcapsules to make same

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US10/377,642 US7192993B1 (en) 2003-03-04 2003-03-04 Self-healing coating and microcapsules to make same
US11/789,811 US20080152815A1 (en) 2003-03-04 2007-02-22 Self-healing coating and microcapsules to make same

Related Parent Applications (1)

Application Number Title Priority Date Filing Date
US10/377,642 Continuation US7192993B1 (en) 2003-03-04 2003-03-04 Self-healing coating and microcapsules to make same

Publications (1)

Publication Number Publication Date
US20080152815A1 true US20080152815A1 (en) 2008-06-26

Family

ID=37863810

Family Applications (2)

Application Number Title Priority Date Filing Date
US10/377,642 Expired - Fee Related US7192993B1 (en) 2003-03-04 2003-03-04 Self-healing coating and microcapsules to make same
US11/789,811 Abandoned US20080152815A1 (en) 2003-03-04 2007-02-22 Self-healing coating and microcapsules to make same

Family Applications Before (1)

Application Number Title Priority Date Filing Date
US10/377,642 Expired - Fee Related US7192993B1 (en) 2003-03-04 2003-03-04 Self-healing coating and microcapsules to make same

Country Status (1)

Country Link
US (2) US7192993B1 (en)

Cited By (17)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20070277948A1 (en) * 2006-05-31 2007-12-06 Usg Interiors, Inc. Acoustical tile
WO2011126165A1 (en) * 2010-04-09 2011-10-13 주식회사 포스코 Organic corrosion inhibitor-embedded polymer capsule, preparation method thereof, composition containing same, and surface treated steel sheet using same
JP2013032419A (en) * 2011-08-01 2013-02-14 Nippon Telegr & Teleph Corp <Ntt> Coating material, and coated film
US20130316083A1 (en) * 2010-11-16 2013-11-28 Akzo Nobel Coatings International B.V. Multipurpose paint formulation
WO2014149741A1 (en) 2013-03-15 2014-09-25 Honda Motor Co., Ltd. Corrosion inhibiting compositions and coatings including the same
WO2015061522A1 (en) * 2013-10-23 2015-04-30 Autonomic Materials, Inc. Self-healing agent formulations containing liquid corrosion inhibitors
US20150174837A1 (en) * 2013-12-19 2015-06-25 General Electric Company Turbine component patch delivery system
US20150174838A1 (en) * 2013-12-19 2015-06-25 General Electric Company Turbine component patch delivery systems and methods
WO2016115348A1 (en) 2015-01-16 2016-07-21 Thomas & Betts International Llc Electrical devices and components used in electrical systems made with self-healing materials
US9404065B2 (en) 2013-01-02 2016-08-02 International Business Machines Corporation Renewable self-healing capsule system
WO2016149148A1 (en) * 2015-03-17 2016-09-22 3M Innovative Properties Company Solventless anti-corrosion composition and methods of using the same
US9550855B2 (en) 2010-05-28 2017-01-24 The Johns Hopkins University Self-healing coatings
US9605162B2 (en) 2013-03-15 2017-03-28 Honda Motor Co., Ltd. Corrosion inhibiting compositions and methods of making and using
CN108191282A (en) * 2018-03-27 2018-06-22 武汉理工大学 One kind is for cement concrete crack autogenous healing polymer emulsion microcapsules and preparation method thereof
WO2018018014A3 (en) * 2016-07-21 2018-07-26 Autonomic Materials, Inc. Peel-resistant self-healing coatings and stains for porous subrtates
CN111925681A (en) * 2020-08-11 2020-11-13 中国船舶重工集团公司第七二五研究所 Anticorrosion and antifouling integrated self-repairing microcapsule and preparation method thereof
US10995236B2 (en) 2015-10-28 2021-05-04 Swimc Llc Polyurethane coating composition

Families Citing this family (31)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6527849B2 (en) * 1990-06-19 2003-03-04 Carolyn M. Dry Self-repairing, reinforced matrix materials
US6518330B2 (en) * 2001-02-13 2003-02-11 Board Of Trustees Of University Of Illinois Multifunctional autonomically healing composite material
US7192993B1 (en) * 2003-03-04 2007-03-20 The United States Of America As Represented By The Secretary Of The Army Self-healing coating and microcapsules to make same
US7566747B2 (en) 2004-05-07 2009-07-28 The Board Of Trustees Of The University Of Illinois Wax particles for protection of activators, and multifunctional autonomically healing composite materials
US7342057B2 (en) * 2004-08-24 2008-03-11 United States Of America As Represented By The Secretary Of The Army Self-healing coatings using microcapsules to suppress lead dust
KR20070086249A (en) * 2004-12-15 2007-08-27 아크조노벨코팅스인터내셔널비.브이. Repair of coated substrates
US7612152B2 (en) * 2005-05-06 2009-11-03 The Board Of Trustees Of The University Of Illinois Self-healing polymers
ES2323386T3 (en) * 2005-06-30 2009-07-14 Bae Systems Plc MATERIALS OF SELF-REPAIR FIBERS AND REPAIR METHODS.
US7811666B2 (en) * 2005-07-01 2010-10-12 Carolyn Dry Multiple function, self-repairing composites with special adhesives
US9227221B2 (en) * 2005-09-19 2016-01-05 The United States Of America As Represented By The Administrator Of The National Aeronautics And Space Administration Hydrophilic-core microcapsules and their formation
US7790225B1 (en) * 2005-09-19 2010-09-07 The United States Of America As Represented By The Administrator Of The National Aeronautics And Space Administration Coatings and methods for corrosion detection and/or reduction
US7723405B2 (en) * 2006-01-05 2010-05-25 The Board Of Trustees Of The University Of Illinois Self-healing coating system
US7569625B2 (en) * 2006-06-02 2009-08-04 The Board Of Trustees Of The University Of Illinois Self-healing elastomer system
US20080299391A1 (en) * 2007-05-31 2008-12-04 White Scott R Capsules, methods for making capsules, and self-healing composites including the same
US20090181254A1 (en) * 2008-01-15 2009-07-16 The Board Of Trustees Of The University Of Illinois Multi-capsule system and its use for encapsulating active agents
CN101818317A (en) * 2010-05-14 2010-09-01 大连海事大学 Metal piece with self-repairing material coating and preparation method thereof
US20130017405A1 (en) * 2010-05-28 2013-01-17 The Johns Hopkins University Self-Healing Coatings
EP2665783A2 (en) 2011-01-19 2013-11-27 President and Fellows of Harvard College Slippery liquid-infused porous surfaces and biological applications thereof
US9353646B2 (en) 2011-01-19 2016-05-31 President And Fellows Of Harvard College Slippery surfaces with high pressure stability, optical transparency, and self-healing characteristics
US8802801B1 (en) 2011-03-25 2014-08-12 Oceanit Laboratories, Inc. Reconfigurable polymeric self-healing coating
CA2878683C (en) 2012-07-12 2021-07-20 President And Fellows Of Harvard College Slippery self-lubricating polymer surfaces
US10011800B2 (en) 2012-07-13 2018-07-03 President And Fellows Of Harvard College Slips surface based on metal-containing compound
US9630224B2 (en) 2012-07-13 2017-04-25 President And Fellows Of Harvard College Slippery liquid-infused porous surfaces having improved stability
US10385181B2 (en) 2013-03-13 2019-08-20 President And Fellows Of Harvard College Solidifiable composition for preparaton of liquid-infused slippery surfaces and methods of applying
US8974259B2 (en) * 2013-03-18 2015-03-10 International Business Machines Corporation Electrical connectors with encapsulated corrosion inhibitor
US9943487B2 (en) 2015-05-26 2018-04-17 The Board Of Trustees Of The University Of Illinois Polydopamine-coated capsules
US10508204B2 (en) 2015-12-02 2019-12-17 The Board Of Trustees Of The University Of Illinois Self-healing coating
CN108912657B (en) * 2018-08-21 2021-04-23 宁波朗茵新材料有限公司 Self-repairing polyurethane cable sheath and preparation method thereof
CN110105843B (en) * 2019-04-30 2020-06-19 中山大学 Stimulus-response self-repairing anticorrosive coating material and preparation method thereof
WO2022073232A1 (en) * 2020-10-10 2022-04-14 深圳烯湾科技有限公司 Self-repairing gas storage tank system and new energy vehicle
CN112547465B (en) * 2020-10-27 2021-12-28 吉林大学 Spraying method of anticorrosive paint for outer surface of marine pipeline of ship

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5575841A (en) * 1990-06-19 1996-11-19 Carolyn M. Dry Cementitious materials
US5660624A (en) * 1990-06-19 1997-08-26 Dry; Carolyn M. Self-repairing, reinforced matrix materials
US6060152A (en) * 1998-08-21 2000-05-09 Murchie; Colin C. Fabric with microencapsulated breach indication coating
US6075072A (en) * 1998-03-13 2000-06-13 3M Innovative Properties Company Latent coating for metal surface repair
US6746522B2 (en) * 1997-11-25 2004-06-08 Gtat, Llc High molecular weight polymer additive for coating and protective products
US7192993B1 (en) * 2003-03-04 2007-03-20 The United States Of America As Represented By The Secretary Of The Army Self-healing coating and microcapsules to make same

Patent Citations (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5575841A (en) * 1990-06-19 1996-11-19 Carolyn M. Dry Cementitious materials
US5660624A (en) * 1990-06-19 1997-08-26 Dry; Carolyn M. Self-repairing, reinforced matrix materials
US5989334A (en) * 1990-06-19 1999-11-23 Dry; Carolyn M. Self-repairing, reinforced matrix materials
US6261360B1 (en) * 1990-06-19 2001-07-17 Carolyn M. Dry Self-repairing, reinforced matrix materials
US6746522B2 (en) * 1997-11-25 2004-06-08 Gtat, Llc High molecular weight polymer additive for coating and protective products
US6075072A (en) * 1998-03-13 2000-06-13 3M Innovative Properties Company Latent coating for metal surface repair
US6060152A (en) * 1998-08-21 2000-05-09 Murchie; Colin C. Fabric with microencapsulated breach indication coating
US7192993B1 (en) * 2003-03-04 2007-03-20 The United States Of America As Represented By The Secretary Of The Army Self-healing coating and microcapsules to make same

Cited By (29)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20070277948A1 (en) * 2006-05-31 2007-12-06 Usg Interiors, Inc. Acoustical tile
WO2011126165A1 (en) * 2010-04-09 2011-10-13 주식회사 포스코 Organic corrosion inhibitor-embedded polymer capsule, preparation method thereof, composition containing same, and surface treated steel sheet using same
US9550855B2 (en) 2010-05-28 2017-01-24 The Johns Hopkins University Self-healing coatings
US20130316083A1 (en) * 2010-11-16 2013-11-28 Akzo Nobel Coatings International B.V. Multipurpose paint formulation
JP2013032419A (en) * 2011-08-01 2013-02-14 Nippon Telegr & Teleph Corp <Ntt> Coating material, and coated film
US9404065B2 (en) 2013-01-02 2016-08-02 International Business Machines Corporation Renewable self-healing capsule system
US10584246B2 (en) 2013-01-02 2020-03-10 International Business Machines Corporation Renewable self-healing capsule system
US10584245B2 (en) 2013-01-02 2020-03-10 International Business Machines Corporation Renewable self-healing capsule system
US10066105B2 (en) 2013-01-02 2018-09-04 International Business Machines Corporation Renewable self-healing capsule system
US10392713B2 (en) 2013-03-15 2019-08-27 Honda Motor Co., Ltd. Corrosion inhibiting compositions and coatings including the same
US11136675B2 (en) 2013-03-15 2021-10-05 Honda Motor Co., Ltd. Corrosion inhibiting compositions and coatings including the same
WO2014149741A1 (en) 2013-03-15 2014-09-25 Honda Motor Co., Ltd. Corrosion inhibiting compositions and coatings including the same
EP3495053A1 (en) 2013-03-15 2019-06-12 Honda Motor Co., Ltd. Corrosion inhibiting compositions
US10988626B2 (en) 2013-03-15 2021-04-27 Honda Motor Co., Ltd. Corrosion inhibiting compositions and methods of making and using
US9605162B2 (en) 2013-03-15 2017-03-28 Honda Motor Co., Ltd. Corrosion inhibiting compositions and methods of making and using
US9816189B2 (en) 2013-03-15 2017-11-14 Honda Motor Co., Ltd. Corrosion inhibiting compositions and coatings including the same
US9279043B2 (en) 2013-10-23 2016-03-08 Autonomic Materials, Inc. Self-healing agent formulations containing liquid corrosion inhibitors
JP2016535820A (en) * 2013-10-23 2016-11-17 オートノミック マテリアルズ、インコーポレイテッド Self-healing agent formulations containing liquid corrosion inhibitors
WO2015061522A1 (en) * 2013-10-23 2015-04-30 Autonomic Materials, Inc. Self-healing agent formulations containing liquid corrosion inhibitors
US10022921B2 (en) * 2013-12-19 2018-07-17 General Electric Company Turbine component patch delivery systems and methods
US20150174838A1 (en) * 2013-12-19 2015-06-25 General Electric Company Turbine component patch delivery systems and methods
US20150174837A1 (en) * 2013-12-19 2015-06-25 General Electric Company Turbine component patch delivery system
WO2016115348A1 (en) 2015-01-16 2016-07-21 Thomas & Betts International Llc Electrical devices and components used in electrical systems made with self-healing materials
WO2016149148A1 (en) * 2015-03-17 2016-09-22 3M Innovative Properties Company Solventless anti-corrosion composition and methods of using the same
US10995236B2 (en) 2015-10-28 2021-05-04 Swimc Llc Polyurethane coating composition
WO2018018014A3 (en) * 2016-07-21 2018-07-26 Autonomic Materials, Inc. Peel-resistant self-healing coatings and stains for porous subrtates
US10519321B2 (en) 2016-07-21 2019-12-31 Autonomic Materials, Inc. Peel-resistant self-healing coatings and stains for porous substrates
CN108191282A (en) * 2018-03-27 2018-06-22 武汉理工大学 One kind is for cement concrete crack autogenous healing polymer emulsion microcapsules and preparation method thereof
CN111925681A (en) * 2020-08-11 2020-11-13 中国船舶重工集团公司第七二五研究所 Anticorrosion and antifouling integrated self-repairing microcapsule and preparation method thereof

Also Published As

Publication number Publication date
US7192993B1 (en) 2007-03-20

Similar Documents

Publication Publication Date Title
US7192993B1 (en) Self-healing coating and microcapsules to make same
US20210214565A1 (en) Corrosion inhibiting compositions and methods of making and using
US11136675B2 (en) Corrosion inhibiting compositions and coatings including the same
US7342057B2 (en) Self-healing coatings using microcapsules to suppress lead dust
US9233394B2 (en) Hydrophobic-core microcapsules and their formation
CN1170893C (en) Latent coating for metal surface repair
US20130017405A1 (en) Self-Healing Coatings
US9227221B2 (en) Hydrophilic-core microcapsules and their formation
JP2002506914A (en) Paint and coating method
Kumar et al. Self Healing Coatings
CN111808521B (en) Self-repairing waterborne polyurethane coating composition and coating
RU2522427C1 (en) Liquid hydroxylamine curing agent for isocyanate prepolymers for producing sprayed polyurea-urethane coatings
EP0096207B1 (en) Water-borne permanent coating compositions and processes therefor
CN112175498A (en) Self-detection water-based self-repairing anticorrosive coating and preparation method thereof
KR102103226B1 (en) Seaside steel structure anticorrosive painting method
RU2805934C1 (en) Anti-corrosion coating to protect inner surface of pipe, composition for its production and method for its production
RU2284342C1 (en) Composition for applying anticorrosive coating
RU2314328C2 (en) Lacquer composition
Beitelman et al. High solids and zinc-rich epoxy coatings for Corps of Engineers civil works structures
Mamat et al. ANTICORROSION PERFORMANCE OF SELF-HEALING POLYMERIC COATING ON LOW CARBON STEEL SUBSTRATES IN 3.5 wt.% NaCl MEDIUM
Mamat et al. A CHARACTERIZATION OF TUNG OIL-FILLED UREA-FORMALDEHYDE MICROCAPSULES AND THEIR EFFECT ON MECHANICAL PROPERTIES OF AN EPOXY-BASED COATING
CN112403409A (en) Self-detection capsule for water-based anticorrosive paint and preparation method thereof
Lyons Topcoat for Military Aircraft
HU193752B (en) Additive compositions improving the quality of enamel paints of alkyd resin type

Legal Events

Date Code Title Description
STCB Information on status: application discontinuation

Free format text: ABANDONED -- FAILURE TO RESPOND TO AN OFFICE ACTION